Influence of samples location and orientation on hot-rolled structural steel mechanical properties: Experimental report

Daniel Carazo-Alvareza,*, Juan J. Jiménez de Cisneros Fonfríab, José Camacho-Sampedroa, Rafael I. Medina Baenaa, Juan de Dios Carazo-Alvareza

aUniversidad de Jaén, Campus “Las Lagunillas”, Building A3, 23071 Jaén, Spain

bAv. Universitaria 1801, San Miguel, Lima 32, Perú

*Corresponding author: dcarazo@ujaen.es

 

ABSTRACT

For an accurate modelling of structures behavior, a precise determination of mechanical properties of structural steel is essential. Mechanical characterization must achieve standard prescriptions; thus, samples must be taken from a specific location and orientation, and the obtained properties from these specimens are used to characterize, uniquely, the steel. The hot-rolling process of structural steel profiles manufacture, which induces residual stresses distribution, can affects to homogeneity and isotropy of final product, therefore, uniformity of mechanical properties along the section is not guaranteed. The variation of these properties depending on orientation and location is studied in this paper. A tensile testing experimental program, where stress – strain curves are recorded and used to obtain mechanical properties at elastic and plastic conditions from different locations and orientations, have been carried out. No similar experimental work was found at literature, except in case of cold-bending formed steel. Results showed no significant differences for most cases, however properties related with necking and failure showed a clear dependence on location. Higher differences were found at specimens from the center of the flange. In addition, the research performed denotes that orientation has no influence on the variation of mechanical properties of hot-rolled steel.

 

RESUMEN

Influencia de la ubicación y orientación de muestras en las propiedades mecánica del acero estructural laminado en caliente: Reporte experimental. Para un modelado adecuado del comportamiento de las estructuras, es esencial una determinación precisa de las propiedades mecánicas del acero estructural. La caracterización mecánica debe satisfacer las prescripciones de las normas; en consecuencia, las muestras deben ser tomadas de una posición y orientación especifica; y las propiedades obtenidas de estos especímenes son usadas para caracterizar, de manera única, el acero. El proceso de laminado en caliente usado en la manufactura de perfiles de acero estructural, que implica la aparición de tensiones residuales, puede afectar a la homogeneidad e isotropía del producto final; por ello, la uniformidad de las propiedades mecánicas a lo largo de la sección no está garantizada. La variación de estas propiedades depende de la orientación y la locación y es estudiada en este artículo. Un programa de ensayos a tracción ha sido llevado a cabo, donde las curvas esfuerzo – deformación son registradas y usadas para obtener las propiedades mecánicas en condiciones elásticas y plásticas desde diferentes posiciones y orientaciones. No se encontraron trabajos experimentales similares en la literatura, excepto en el caso de acero conformado por doblado en frío. Los resultados no muestran diferencias significativas en la mayoría de casos; no obstante, las propiedades relacionadas con la estricción y falla muestran una clara dependencia con la ubicación. Las diferencias más importantes se hallaron en las muestras localizadas en el centro del ala; además, la investigación realizada denota que la orientación no influye en la variación de las propiedades mecánicas del acero laminado en caliente.

 

Submitted: 28 October 2019; Accepted: 20 January 2020; Available On-line: 20 July 2020

Citation/Citar como: Carazo-Alvarez, D.; Jiménez de Cisneros Fonfría, J.J.; Camacho-Sampedro, J.; Medina Baena, R.I.; Carazo-Alvarez, J. (2020). “Influence of samples location and orientation on hot-rolled structural steel mechanical properties: Experimental report”. Rev. Metal. 56(1): e162. https://doi.org/10.3989/revmetalm.162

KEYWORDS: Mechanical testing; Plastic deformation; Standard; Structural steel; Tensile properties

PALABRAS CLAVE: Acero estructural; Caracterización mecánica; Deformación plástica; Estándares; Propiedades en tracción

ORCID ID: Daniel Carazo-Alvarez (https://orcid.org/0000-0002-8909-1863); Juan J. Jiménez de Cisneros Fonfría (https://orcid.org/0000-0002-8464-9581); José Camacho-Sampedro (https://orcid.org/0000-0003-3772-1373); Rafael I. Medina Baena (https://orcid.org/0000-0003-2889-8249); Juan de Dios Carazo-Alvarez (https://orcid.org/0000-0002-1532-2550)

Copyright: © 2020 CSIC. This is an open-access article distributed under the terms of the Creative Commons Attribution 4.0 International (CC BY 4.0) License.


 

CONTENT

1. INTRODUCTIONTOP

A fair determination of the mechanical properties of structural steel is essential for an accurate modeling of the behavior of a structure. Standards supply values for yield and ultimate strength for each type of steel, in conjunction with general values for the Young’s modulus and the Poisson’s ratio. These values are enough to carry out the structural design, however, values of other mechanical properties as: hardening modulus, fracture strength or fracture strain, which are required to predict the behavior under unusual load conditions, are not included at standards, and must be experimentally determined.

In Europe, two standards must be taken into account when designing the experimental program for determining such properties, i.e. ISO 377 (2017), which is used for location and preparation of specimens, and ISO 6892-1 (2016), which establishes the procedure for tensile testing. The ASTM A370-16 (2016) agrees with them for the most important issues. The first one assumes that, as a result of manufacturing process, steel products are heterogeneous, so the mechanical properties of samples from various locations can be different. Even more, in the case of hot-rolled beams, steel from webs and from flanges must be considered as different steels. According to this, specimens must be obtained from a specific location and orientation, depending on: the final use of the product (beams, bars, plates, etc.), the geometry and the thickness. Specimens must be located at the center of the piece and away from the edge, where properties can be disrupted by the manufacturing process. Orientation must be coincident with the shape rolling axis. This carries a significant material loss, as explained ahead in this paper.

Mechanical properties of steel can be used in different types of simulations, such as those using the Finite Element Method (FEM), or those obtained from theoretical or parametric models. FE software typically allows a complete description of the stress – strain curve, whereas theoretical and parametrical models commonly require, uniquely, the values of the main properties, as in Piluso et al. (2001) and Coelho et al. (2004). In all these simulations, it is assumed that the properties are the same at every point of the structure than those obtained by testing samples from a specific part.

Those main mechanical properties are obtained from engineering stress – strain curves, as coordinates of several significant points. ISO 6892-1 (2016), establishes the procedure for obtaining some of these properties. The remaining properties are usually obtained from true stress – strain curves, which can be drawn from the engineering one.

The aim of this paper is to determine the difference between mechanical properties of specimens obtained from different locations and orientations of the flanges of a structural steel hot-rolled beam. An experimental program consisting of tensile testing of specimens from different locations, orientations and cross-section has been carried out. Strain gages have been used to obtain accurate strain measurements. The stress – strain curves (engineering and true) have been represented, and mechanical properties were obtained and compared from these curves. Results are not homogeneous and some interesting conclusions are drawn below.

2. MATERIALS AND METHODSTOP

2.1. Basis & standards prescriptionsTOP

A stress-strain curve can be described by a few essential points and slopes where trend changes. Specifically, these points are (Fig. 1):

Figure 1. Essential points at stress – strain curves for structural steel.

 
A.  End of elastic behavior, which is defined by yield strength fy (stress at point A) and Young Modulus E (slope of line 0-A). Determination of fy is typically done by means of the 0,2% offset method.
B.  End of yielding, usually estimated as a flat behavior, defined by means of strain at the beginning of hardening εh (strain at B).
C.  End of strain hardening, or maximum load point, usually defined by ultimate strength fu and ultimate strain εu, and also by means of the hardening modulus Eh (average slope of section B-C).
D.  Fracture, defined by fracture strength ff and fracture strain εf (coordinates of D). Necking phase is defined by means of the necking modulus Eu (average slope of section C-D).

These properties are obtained from the engineering stress-strain curve, however, several approaches (Piluso et al., 2001; Coelho et al., 2004) uses values obtained from the true stress – strain (C’ and D’ shown at Fig.1). True stress-strain curves can be drawn from engineering curves by applying Nadai’s equations (Nadai, 1933):

where ft and et are stress and strain at the true curve obtained from f and ε at the engineering curve.

For commonly used structural steels, reference values of these properties can be found at literature (Kato et al., 1990; Gioncu and Mazzolani, 2002). These values have been summarized at Table 1. Also, the ISO 6892-1 (2016), defines additional properties related to the specimen dimensions after failure, actually:

Table 1. Mechanical properties reference values for structural steels from (Kato et al., 1990; Gioncu and Mazzolani, 2002)
Steel fy [N·mm-2] fu [N·mm-2] εy [%] εh [%] εu [%] εf [%] Eh [N·mm-2] Eu [N·mm-2]
S235 235 360 0.115 1.41 14.0 25.0 5500 360
S275 275 430 0.134 1.47 12.0 22.0 4800 430
S355 355 510 0.173 1.70 11.0 20.0 4250 510
–  The percentage elongation after fracture A, is defined as the permanent elongation of the gauge length after fracture, expressed as a percentage of the original gauge.
–  The percentage reduction of area Z, is defined as the maximum change in cross-sectional area which has occurred during the test, expressed as a percentage of the original cross-sectional area.

However, structural steel must meet the requirements of the corresponding national regulation in terms of elastic limit and resistance. In Europe, most countries apply values suggested at Eurocode 3 (EN 1993-1-1, 2005). which also depend on the nominal thickness of the element. As ductility requirements, the Eurocode 3 (EN 1993-1-1, 2005) recommends these conditions for fu and εu:

Design values for Young’s modulus and Poisson’s ratio are also shown, but no conditions to other properties like hardening strain εh, hardening modulus Eh, necking modulus Eu or fracture stress ff are established at Eurocode 3 (EN 1993-1-1, 2005).

ISO 377 (2017) establishes that, for flange rolled beam steel, location of samples across the width of section must be 1/3 away from edges and 2/3 away from center of section, as shown in Fig. 2a. About the location in thickness of section, full thickness samples must be used (Fig. 2.b). Given that circular or rectangular cross-section test pieces can be machining from these samples, only the rectangular one will finally keep the full thickness, so cross-section may also have some influence on results, as discussed by RILEM (1990) orientation of test tubes must be the same as shape rolling axis. The influence of these prescriptions on the mechanical properties has been highlighted as the main subject of this research.

Figure 2. Location of test pieces across the width of section (a) and in thickness of section (b) from (ISO 377, 2017).

 

The hot rolling manufacturing process results in a recrystallization of steel, which might happen in static or dynamic conditions, and with temperature playing a very important role. Cooling rate along shape rolling axis is lower than along radial direction. thus, grain growth is not isotropic, mainly in the presence of some elements such as Nickel or Chromium (Llewellyn and Hudd, 1998; Lenard et al., 1999). However, hot rolling is not a strengthening process itself, therefore great differences at mechanical properties values are not expected.

Test tube locations are chosen by the standard look away from areas prone to unrepresentative defects such as edge defects, in order to improve the quality of the sample’s representation. Moreover, the manufacturing process is affected by several chemical, mechanical and thermal parameters; thus, some mechanical property predictions models were proposed considering these parameters (Zhao et al., 2013), although no experimental studies about the influence of location and orientation have been found. Similar works have been previously carried out by Spoorenberg et al. (2012), in the field of cold-bending formed steel.

2.2. Experimental programTOP

In order to verify if ISO 377 (2017) prescriptions about location of samples have any influence on the mechanical properties, forty-two test tubes were tensile strength tested, obtaining significant readings for thirty-six of them, and dismissing the results of six due to out of range results. Variables of interest are: location across the width, orientation and cross-section shape.

Four different location/orientation and two different shapes of specimens were selected, as detailed in Table 2 and Fig. 3. All of them were obtained from the flanges of an HEB400 beam of S275 structural steel. Dimensions of specimens are shown at Fig. 4. These dimensions are chosen to meet ISO 6892-1 (2016) requirements.

Table 2. Description of tested specimens and corresponding batch (amount of specimens between brackets)
Specimens Cross-section Location / orientation Batch ID
Total (36) Rectangular (18) At L/3 (5) A
    At L/2 (4) B
    At L (in the center) (4) C
    Transverse orientation (5) D
  Circular (18) At L/3 (4) E
    At L/2 (4) F
    At L (in the center) (4) G
    Transverse orientation (6) H

Figure 3. Location of specimen batches: A. B. C and D with rectangular cross-sections and E. F. G y H with circular cross-sections.

 

Figure 4. Dimensions of specimens with rectangular (a) and circular (b) cross-section (mm).

 

The preparation of specimens is carried out in two main phases: First, the right prism from the flanges of the beam with the location and orientation intended is obtained by wheel sawing, band sawing and oxycutting. Later, the bone shape with the final dimensions is achieved by using numerical control milling and turning, which also serves to remove the oxycutting heat affected zone. Final dimensions of specimens meet tolerance limits indicated at ISO 6892-1 (2016).

Obviously, steel properties are related to constituent elements and their percentage. In the case of structural steels, standard values are used to establish percentage limits or range for each element.

Before tensile testing of the specimens, an inductively coupled plasma mass spectrometry (ICP-MS) was used in order to obtain the steel composition and verify compliance with the standard. Six samples were prepared following the ISO 14284 (1996) and results (Table 3) showed that Carbon, Nitrogen, Hydrogen and Sulfur contents meet the EN 10025-2 (2004).

Table 3. Steel chemical composition obtained with ICP-MS
Sample Nitrogen % Carbon % Hydrogen % Sulfur %
1 0.0096 0.1123 0.0036 0.0099
2 0.0076 0.1159 0.0023 0.0084
3 0.0026 0.1101 0.0032 0.0000
4 0.0021 0.1016 0.0029 0.0000
5 0.0015 0.0962 0.0016 0.0000
6 0.0016 0.0935 0.0016 0.0000
average 0.0042 0.1049 0.0025 0.0030

Post-yield foil strain gages are employed to perform strain measurements, due to their high accuracy. A cyanoacrylate adhesive (CN-Y, Tokyo Sokki Kenkyujo Co.) is used, since it is suitable for post-yield behavior. Finally, strain was read from the gages by a P3 Strain Indicator (Vishay Micro-Measurements Co.-Wendell, NC, USA).

Tensile testing was carried out using a MTS 810 loading machine, of 100 kN load capacity. Load was applied at the rate of 0.5 mm·min-1, within the range suggested by standard. Extensometers were also used to validate strain gages measurement.

3. RESULTSTOP

Stress-strain curves have been drawn for each specimen tested based on readings from strain gages and load cells.

These curves are shown at Fig. 5. Also, average curves were obtained for each batch by applying regression to three separate portions of the curves, as follows:

Figure 5. Stress – strain curves obtained for each specimen. and average curves (dashed lines) calculate per batch.

 
–  Linear regression at the elastic region (y = Ex, where E is the Young modulus).
–  6th degree polynomial regression at yielding (y = ax6 + bx5 + cx4 + dx3 + ex2 + fx + g), and also,
–  6th degree polynomial regression at the plastic region.

Average coefficients for regressions at elastic, yielding and plastic regions are shown at Table 4 for each batch. A minimum correlation factor of 0.99 was set as objective when performing the regression analysis for each specimen. After several attempts, 6th degree functions are required to achieved the desired correlation factor.

Table 4. Regression coefficients for batch average stress – strain curves
  Batch
A B C D E F G H
Yielding a 36.86 -0.63 0.02 -10.36 2768.77 5228.53 4106.48 -623.70
  b -295.41 -3.07 4.53 85.31 -10057.76 -17729.41 -15055.94 1830.91
  c 949.01 26.92 -21.55 -272.83 15078.15 24137.95 21516.67 -1538.23
  d -1555.07 -61.84 39.53 435.32 -11664.48 -16644.51 -15094.05 -143.51
  e 1364.02 66.30 -35.09 -367.80 4730.60 6016.82 5429.46 788.88
  f -600.51 -28.09 17.89 161.23 -912.46 -1056.40 -942.48 -348.52
  g 424.64 305.15 315.48 287.75 357.49 359.89 331.17 324.26
Plastic a -1,00E-04 -6,07E-05 -5,68E-05 -6,54E-05 -1,63E-05 -6,81E-05 -4,79E-05 -5,39E-05
  b 8,80E-03 4,25E-03 3,98E-03 4,84E-03 1,21E-04 3,53E-03 1,90E-03 2,72E-03
  c -2,33E-01 -1,21E-01 -1,14E-01 -1,46E-01 1,18E-02 -7,32E-02 -3,26E-02 -5,68E-02
  d 3.22 1.82 1.72 2.33 -0.20 0.84 0.41 0.70
  e -25.28 -15.75 -15.19 -21.24 -0.41 -6.84 -5.08 -6.69
  f 116.75 83.28 83.06 114.13 26.88 45.79 45.45 49.49
  g 156.65 188.18 206.84 123.42 286.93 270.43 256.56 250.63

Finally, mechanical properties have been obtained for each specimen, and average values and standard deviation σ calculated for each batch of specimens. Results are shown at Table 5. Properties are divided into three categories:

Table 5. Mechanical properties obtained for every specimen. and batch’s average values
  Basic properties True properties Standard properties
E fy fu εh Eh εu ff εf Eu A Z
[N·mm-2] [%] [N·mm-2] [%] [N·mm-2] [%] [N·mm-2] [%] [%]
A1 200834 232 438 1.51 1300 17.00 474 19.81 474 21.91 40.23
A2 197677 284 436 1.39 1141 17.45 464 20.56 464 22.83 39.08
A3 247546 339 448 1.62 1309 15.79 448 19.11 448 21.06 43.55
A4 211931 328 448 1.83 1421 14.83 408 17.83 408 19.51 37.62
A5 212090 270 433 1.50 1183 16.39 387 19.91 387 22.03 44.38
214016 291 441 1.57 1271 16.29 436 19.44 436 21.47 40.97
σA 9.27% 15.0% 1.6% 10.6% 8.7% 6.3% 8.5% 5.3% 8.5% 5.9% 7.1%
B1 185567 242 385 1.64 1061 17.52 388 20.89 -1953 23.06 43.14
B2 214217 312 437 1.71 1255 18.22 426 21.96 -2457 24.39 40.57
B3 194330 276 450 1.63 1467 14.12 453 17.47 -1866 20.16 43.98
B4 235742 293 427 1.39 1190 17.31 419 20.84 -2354 23.02 44.18
207464 281 425 1.59 1243 16.79 422 20.29 -2158 22.66 42.97
σB 10.8% 10.6% 6.6% 8.8% 13.6% 10.9% 6.3% 9.6% -13.5% 7.9% 3.9%
C1 204943 332 459 1.45 1194 16.79 474 20.20 -1815 21.98 44.54
C2 197491 282 447 1.58 1398 16.82 471 20.09 -1630 22.06 43.80
C3 209935 299 443 1.31 1669 9.51 - - - - -
C4 212828 322 442 1.67 1193 16.91 423 20.46 -2685 22.54 39.77
206299 309 448 1.50 1364 15.01 456 20.25 -2043 22.19 42.70
σC 3.3% 7.3% 1.7% 10.4% 16.5% 24.4% 6.3% 0.9% -27.6% 1.4% 6.0%
D1 209256 328 443 1.91 1220 18.41 448 22.25 -2047 24.74 45.96
D2 173588 288 432 - 1318 18.15 447 21.36 -2053 23.61 47.78
D3 185799 287 439 1.59 1308 17.49 453 20.62 -2099 22.71 41.37
D4 213740 327 449 1.46 1400 16.52 477 19.34 -1681 21.15 39.99
D5 232174 289 435 1.72 1290 17.17 454 20.02 -2042 22.00 37.87
202911 304 440 1.67 1307 17.55 456 20.72 -1984 22.84 42.59
σD 11.5% 7.1% 1.5% 11.5% 4.9% 4.3% 2.7% 5.5% -8.6% 6.1% 9.7%
E1 216351 296 438 1.12 1644 14.04 390 17.40 -3309 20.50 45.79
E2 214669 290 441 1.02 1419 16.37 364 20.43 -3766 20.75 67.30
E3 217252 301 443 1.04 1365 14.70 358 18.21 -4311 28.75 68.32
E4 210939 300 443 1.13 1459 14.74 365 18.80 -3581 20.25 66.37
214803 297 441 1.08 1472 14.96 369 18.71 -3742 22.56 61.95
σE 1.3% 1.7% 0.5% 5.2% 8.2% 6.6% 3.8% 6.9% -11.3% 18.3% 17.4%
F1 212435 295 438 0.94 1731 15.30 - - - - -
F2 207123 288 440 0.96 1531 15.43 360 19.43 -3735 52.50 67.23
F3 218752 296 442 1.03 1414 15.46 637 18.68 -4478 29.00 66.88
F4 220152 287 439 0.97 1296 15.07 414 18.21 -2959 30.00 56.15
214616 292 440 0.98 1493 15.32 470 18.77 -3724 37.17 63.42
σF 2.8% 1.6% 0.4% 4.0% 12.4% 1.2% 31.2% 3.3% -20.4% 35.8% 9.9%
G1 192057 274 440 - 1895 12.87 356 16.06 -4417 29.00 66.53
G2 215994 273 439 1.01 1654 15.20 358 19.19 -3774 33.50 67.43
G3 212979 267 433 0.84 1430 14.75 351 18.22 -4225 33.50 66.25
G4 212125 272 432 0.96 1451 14.63 349 18.48 1451 28.75 67.09
208289 272 436 0.94 1608 14.36 354 17.99 -2741 31.19 66.83
σG 5.3% 1.1% 0.9% 9.3% 13.5% 7.1% 1.2% 7.5% -102% 8.6% 0.8%
H1 210229 284 437 1.04 1330 15.53 373 18.88 -3967 54.75 63.49
H2 220176 284 438 1.06 1378 15.40 368 18.87 -3971 32.00 64.34
H3 209550 287 439 0.93 1372 15.04 379 18.50 -3642 64.50 64.41
H4 212675 285 439 1.07 1260 15.22 368 19.02 -3687 28.75 64.34
H5 209412 261 434 1.35 1689 14.82 368 18.27 -3829 26.00 63.77
H6 206335 267 434 1.19 1654 15.15 381 18.75 -3369 30.00 63.84
211396 278 437 1.11 1447 15.19 373 18.72 -3744 39.33 64.03
σH 2.2% 4.0% 0.5% 13.1% 12.4% 1.7% 1.6% 1.5% -6.1% 41.0% 0.6%
–  Basic properties, which are acquired from the engineering stress – strain curves.
–  True properties, obtained from the true stress – strain curves, drawn by using Eq. (1).
–  Standard properties, as defined at ISO 6892-1 (2016) and related to specimen dimensions after failure.

4. DISCUSSIONTOP

The results listed in Table 5 and illustrated in Fig. 5 exhibit a high degree of similarity. However, a detailed comparison of average curves and calculated properties is required in order to identify differences due to location, orientation and cross-section of test tubes along the flange of the beam.

A first comparison between results obtained at the same location and orientation, but with different cross-sections is carried out. Hence, results from batches A (rectangular) and E (circular) are compared. Both batches are located at L/3 from the edge of the flange and follow standard prescriptions about location and orientation. Figure 6 shows A and E batches average curves and Table 6 has a comparison of calculated properties for each batch. Only properties related with necking and failure conditions show significant differences. Standard deviation values show that most properties values are steady, except necking modulus Eu. The obtained mechanical properties meet the Eurocode 3 (CEN/TC 250 (EN 1993-1-1, 2005)) requirements related to fy, fu and Eq. (2). Values are also similar to those cited at Table 1 from bibliography, except in case of hardening modulus Eh and necking modulus Eu. The hardening modulus Eh is far away from the values reported at Table 1, and results show a Eh close to 0.35 times the given value at references. The necking modulus Eu obtained for rectangular specimens is only a 1,4% away from the value of Table 1, however, the one obtained for circular cross-section specimens has a much higher difference.

Table 6. Mechanical properties comparison for A and E batches
  Basic properties True properties Standard properties
E fy fu εh Eh εu ff εf Eu A Z
[N·mm-2] [N·mm-2] [N·mm-2] [%] [N·mm-2] [%] [N·mm-2] [%] [N·mm-2] [%] [%]
214016 291 441 1.57 1271 16.29 436 19.44 436 21.47 40.97
σA 9.27% 15.0% 1.6% 10.6% 8.7% 6.3% 8.5% 5.3% 8.5% 5.9% 7.1%
214803 297 441 1.08 1472 14.96 369 18.71 -3742 22.56 61.95
σE 1.3% 1.7% 0.5% 5.2% 8.2% 6.6% 3.8% 6.9% -11.3% 18.3% 17.4%
214409 294 441 1.32 1371 15.63 403 19.08 -1653 22.02 51.46
σAE 0.3% 1.5% 0.1% 26.3% 10.4% 6.0% 11.8% 2.7% -178% 3.5% 28.8%

Figure 6. Stress – strain average curves comparison for batches A and E.

 

Comparison of the remaining batches is performed taking the average values of A and E batches as reference. Differences are shown in Table 7, where it can be seen that, for rectangular cross-section specimens (batches B, C and D), the differences are maintained below about 10%, except for three values: strain at hardening εh, necking modulus Eu and percentage reduction of area Z. Figure 7 shows the stress-strain curves for all these batches. It can be seen that the curve obtained for the middle of the flange (batch C) are the least approaching the reference curve of standards (batch A), similar to conclusions with cold-bending formed steel (Spoorenberg et al., 2012).

Table 7. Percentage differences founded in mechanical properties per batch. using AE mean values as reference
  Basic properties True properties Standard properties
E fy fu εh Eh εu ff εf Eu A Z
Dif. -3.2 -4.4 -3.7 20.3 -9.3 7.5 4.7 6.4 30.5 2.9 -16.5
Dif. -3.8 5.1 1.5 13.5 -0.6 -4.0 13.2 6.1 23.6 0.8 -17.0
Dif. -5.4 3.4 -0.3 26.2 -4.7 12.3 13.2 8.6 20.1 3.8 -17.2
Dif. 0.1 -0.7 -0.3 -26.3 8.9 -2.0 16.8 -1.6 125.3 68.8 23.2
Dif. -2.9 -7.6 -1.1 -29.2 17.2 -8.1 -12.2 -5.7 65.9 41.7 29.9
Dif. -1.4 -5.3 -0.9 -16.4 5.5 -2.8 -7.4 -1.9 126.5 78.7 24.4

Figure 7. Stress – strain average curves comparison for batches with rectangular cross-section A. B. C and D.

 

Similar differences can be found when analyzing results obtained for circular cross-section specimens (batches F, G and H), although, in this case, the percentage elongation after fracture A also shows differences over 20%. Figure 8 shows the curves for all circular cross-section batches. Again, the least approaching the reference curve is the specimen from the center of the flange (batch G).

Figure 8. Stress – strain average curves comparison for batches with circular cross-section E. F. G and H.

 

Finally, results obtained from specimens with transverse orientation (batches D and H) do not show a differentiated behavior from those specimens with longitudinal orientation. Further work about the isotropy of hot rolled steel is required, since the confirmation of this premise can generate a very important material saving, which can reach 80%, as performed in this study. Figure 9 shows the HEB400 beam flanges ready for longitudinal and transverse samples extraction, where the difference in the length of beam required for obtaining the specimens can be seen.

Figure 9. Beam flanges ready for longitudinal and transverse samples extraction.

 

5. CONCLUSIONSTOP

–  A total amount of 42 specimens with different locations, orientations and cross-sections, have been tensile-tested in order to quantify the variation of eleven mechanical properties. Experimental data have been used to draw engineering and true stress - strain curves for every specimen tested. Batch average curves have been obtained by means of three polynomic regressions (applied to three parts of the curve). Average curves and values were finally used for discussion of experimental results.
–  Most curves compared are very similar and the main differences are shown at necking and failure behavior. Specimens extracted from the middle of the flange less approaches reference curves (at L/3, as standard states). Mechanical properties values are very similar in most cases, except for necking modulus Eu. About differences between cross-sections, rectangular and circular specimens also differ in percentage reduction of area Z and strain at hardening εh. Specimens with transverse orientation do not show significant differences from the reference, so the isotropy of steel is not very affected by the manufacturing process. The obtained mechanical properties achieve the Eurocode 3 CEN/TC 250 (EN 1993-1-1, 2005) prescriptions and are also similar to those found at literature.
–  Despite limitations of experimental program, it can be said that mechanical properties of a structural steel do not change significantly for different locations and orientation than those state at standard. Main differences were found at the middle of the flange, and for necking and failure properties.

 

REFERENCESTOP


ASTM A370-16 (2016). Standard test methods and definitions for mechanical testing of steel products. Conshohocken, Pennsylvania, California, USA. https://www.astm.org/DATABASE.CART/HISTORICAL/A370-16.htm.
Coelho, A.M.G., Da Silva, L.S., Bijlaard, F.S.K. (2004). ­Characterization of the nonlinear behaviour of single bolted T-Stub connections. Proceeding of Connections in Steel Structures V, Amsterdam, Netherlands, pp. 53–64. https://www.steel.org.au/resources/elibrary/library-items/characterization-of-the-nonlinear-behaviour-of-sin/.
EN 10025-2 (2004). CEN/ECISS/TC103: Hot rolled products of structural steels – Part 2: Technical delivery conditions for non-alloy structural steels. European Committee for Standardization. Brussels, Belgium. https://standards.cen.eu/dyn/www/f?p=204:110:0::::FSP_PROJECT,FSP_ORG_ID:19742,734438&cs=19ED055BD7D76C04289651731E88EAB05.
EN 1993-1-1 (2005). CEN/TC 250, Eurocode 3: Design of steel structures - General rules and rules for building. European Committee for Standardization. Brussels, Belgium. https://standards.cen.eu/dyn/www/f?p=204:110:0::::FSP_PROJECT:12454&cs=11B4D194E5706FD8900424D5E375E9801.
Gioncu, V., Mazzolani, F. (2002). Ductility of Seismic-resistant Steel Structures. CRC Press, United Kingdom. https://www.crcpress.com/Ductility-of-Seismic-Resistant-Steel-Structures/Gioncu-Mazzolani/p/book/9780419225508.
ISO 14284 (1996). ISO/TC17/SC1, Steel and iron: Sampling and preparation of samples for the determination of chemical composition. International Organization for Standardization, Switzerland. http://www.iso.org/iso/catalogue_detail.htm?csnumber=24063.
ISO 6892-1 (2016). ISO/TC164/SC1, Metallic materials – Tensile testing – Part 1: Method of test at room temperature. International Organization for Standardization, Switzerland. https://www.iso.org/standard/61856.html.
ISO 377 (2017). ISO/TC17/SC20, Steel and steel products - Location and preparation of samples and test pieces for mechanical testing. International Organization for Standardization, Switzerland. https://www.iso.org/standard/72529.html.
Kato, B., Aoki, H., Yamanouchi, H. (1990). Standardized mathematical expression for stress-strain relations of structural steel under monotonic and uniaxial tension loading. Mater. Struct. 23, 47–58. https://doi.org/10.1007/BF02472997
Lenard, J.G., Pietrzyk, M., Cser, L. (1999). Chapter 6 - Microstructure Evolution and Mechanical Properties of the Final Product. In: Mathematical and Physical Simulation of the Properties of Hot Rolled Products. Elsevier Science, pp. 151–236. https://doi.org/10.1016/B978-008042701-0/50006-1.
Llewellyn, D.T., Hudd, R.C. (1998). Low-carbon structural steels. In: Steels: Metallurgy and applications. Chapter 2, Hudd DTLC (Ed), Butterworth-Heinemann, Oxford, pp. 137–198. https://doi.org/10.1016/B978-075063757-2/50002-0.
Nadai, A. (1933). Theories of Strength. J. Appl. Mech. 1, 111–129.
Piluso, V., Faella, C, Rizzano, G. (2001). Ultimate behavior of bolted T-Stubs. I: Theoretical model. J. Struct. Eng - ASCE 127 (6), 686–693. https://doi.org/10.1061/(ASCE)0733-9445(2001)127:6(686).
RILEM (1990). Tension testing of metallic structural materials for determining stress-strain relations under monotonic and uniaxial tensile loading. RILEM Draft Recommendation, Mater. Struct. 23, 35–46. https://doi.org/10.1007/BF02472996.
Spoorenberg, R.C., Snijder, H.H., Hoenderkamp, J.C.D. (2012) Mechanical properties of roller bent wide flange sections — Part 1: Experimental investigation. J. ­Constr. Steel Res. 68 (1), 51–62. https://doi.org/10.1016/j.jcsr.2011.07.003.
Zhao, Y., Weng, Y., Peng, N., Tang, G.B., Liu, Z.D. (2013). ­Prediction of Mechanical Properties of Hot Rolled Strip by Using Semi-Parametric Single-Index Model. J. Iron Steel Res. Int. 20, 9–15. https://doi.org/10.1016/S1006-706X(13)60119-3.